PPSU

1 Polyphenylsulfone 

Note

PPSU and its filled carbon fiber version are classified as experimental materials for advanced users.

Info

While you are free to use any brand and type of material you wish on your AON3D machine, we can only provide support for AON3D-approved materials that we have tested and developed processes for in-house, all of which can be purchased from AON3D directly by contacting sales@aon3d.com.

1.1 General Process Settings

SettingValue
Extrusion Temperature340-395ºC
Bed Temperature150-160ºC
Chamber Temperature110ºC

1.2 Usage Notes

1.2.1 Build Surface Preparation

PPSU prints best on the AON-M2 High-Temperature Build Plate with the use of a brim or raft. Note that PEI surface of the High-Temperature Build Plate should be periodically resurfaced using a mill, or with an orbital palm sander if no milling services are available.

Please contact sales@aon3d.com if you currently have an AON-M2 Aluminum Build Plate and would like to upgrade to the AON-M2 High-Temperature Build Plate.

1.2.2 Material Pre-treatment

PPSU is susceptible to moisture uptake. We recommend drying the filament overnight at 120ºC before use, and to always store in a sealed container with desiccant.

Take care to check the spool material of your filament prior to baking your material. Some vendors use low temperature materials for spools which may melt or deform at bakeout temperature.

Please contact support@aon3d.com for any questions on this matter.

1.2.3 Support Material

There is currently no compatible support material for PPSU - prints will require self-support.


1.3 Sample Slicer Profiles

Single Extruder, 0.6mm nozzle: ppsu-sx-0.6mm